Why a sealed unit mists: the desiccant, the seal and the pressure cycle

A sealed unit mists when the primary edge seal thins, the daily pressure cycle pumps damp air into the cavity and the desiccant finally saturates.

How a sealed unit fails and mistsA sealed unit holds dry air or argon between two panes, kept dry by desiccant in the spacer bar. Daily heating and cooling pumps the cavity; once the edge seal loses its grip, moist air is drawn in, the desiccant saturates, and the misting that appears between the panes cannot be cleaned because it is on the inside.cavity: dry air or argonspacer with desiccantedge sealmisting sits between the panes, so it cannot be cleaned offmoist air

A sealed unit does not mist because the glass has worn out. Glass does not wear out. It mists because a seal a few millimetres wide has stopped keeping water vapour on the outside, and the small charge of desiccant that was quietly buying time has finally run out of appetite.

Almost every conversation about a cloudy skylight starts with the pane and should start with the perimeter. The two sheets of glass in a rooflight are, in engineering terms, the least interesting part of it. What decides how long the unit lasts is a narrow band of sealant and a strip of perforated aluminium or polymer hidden behind the frame, where nobody can see it and nobody ever inspects it. This guide is about what is happening in that band, because once you understand the mechanism you can tell a unit that failed early from one that simply finished, and the two lead to different replacements.

What is actually inside the sandwich

A sealed unit, or insulating glass unit, is an assembly rather than a product. Six components do six jobs, and five of them are invisible once the rooflight is glazed.

Component What it does How it fails
Outer and inner panes Carry wind, snow and impact load and hold the low-emissivity coating Rarely. Breakage aside, the panes normally outlive everything around them
Cavity gas Slows conduction and convection across the gap Permeates slowly out through the secondary seal, year on year
Spacer bar Holds the panes apart at a fixed distance and carries the desiccant A plain aluminium bar conducts heat around the edge and makes the cold strip worse
Desiccant Adsorbs the small amount of moisture sealed in at manufacture, and anything that creeps in afterwards Saturates. It has a fixed capacity and no way to regenerate
Primary seal A thin bead of polyisobutylene between spacer and glass. The actual vapour barrier Loses adhesion or thins out under repeated movement, letting damp air past
Secondary seal Structural. Holds the sandwich together and protects the primary seal Degrades under ultraviolet or loses elasticity, which then overloads the primary seal

Two seals, then, doing two unrelated jobs. That distinction is the whole subject, and it is the reason a rooflight specified as a window mists early.

The desiccant is a countdown, not a cure

When a unit is made, the air or gas sealed inside it carries a little moisture. The desiccant packed into the spacer bar adsorbs that moisture and drops the dew point inside the cavity to something far below any temperature the glass will ever reach. A new unit will not mist because the air inside it is drier than any night in Dorset.

The desiccant has a fixed capacity. Nothing regenerates it, and no service can. Every molecule of water vapour that finds its way past the primary seal is permanently spent capacity. For years this is invisible, because the desiccant is winning. Then it saturates, and from that day the dew point inside the cavity rises steeply, because there is nothing left holding it down. This is why a unit appears to fail overnight after twenty uneventful years. The failure took most of those years. Only the symptom was sudden.

The pressure cycle that does the pumping

A sealed cavity is not at a constant pressure. It is pumped, twice a day, every day, by the weather.

  1. Morning sun strikes the outer pane. The gas in the cavity warms and expands, and because the panes are fixed at the perimeter, the only place the expansion can go is outwards. Both panes bow away from each other by a fraction of a millimetre.
  2. That bowing puts the primary seal into tension and the secondary seal into shear. It is a small movement and an enormous number of repetitions.
  3. Late afternoon the glass cools. The gas contracts and the panes bow inwards, reversing the load on both seals.
  4. Overnight, radiative cooling to a clear sky pulls the outer pane below air temperature, which exaggerates the contraction well beyond what the day’s high suggested.
  5. Barometric pressure moves independently of all of that. A deep low crossing the Channel changes the pressure differential across the seal for days at a time.
  6. Where the primary seal has thinned, each cycle draws a breath of damp outside air in and pushes a breath of dry cavity air out. The desiccant takes the water. The countdown accelerates.

A rooflight sees a bigger swing than a wall window on the same house, because it faces the sky rather than the horizon. It gets the full solar load in summer and the full radiative loss on a clear winter night, and the daily excursion at the glass line is correspondingly wider.

Two seals, two different jobs

The rule, and the exception that matters overhead

The rule. The primary seal keeps vapour out and has almost no mechanical strength. The secondary seal has the strength and keeps the primary seal in place. If the secondary seal degrades, the primary seal is left carrying loads it was never designed for, and it fails soon afterwards.

The exception. The usual secondary sealant on a volume-made window unit is polysulphide. It is durable, cheap and it does not like ultraviolet. In a vertical window it barely sees any, because the frame covers the edge and the sun arrives at a shallow angle. In a rooflight the sun is overhead for months, the edge cover is often shallower, and a slimline frame can leave the perimeter seal effectively sunbathing. For overhead and structurally bonded glazing the secondary seal should be silicone, which is ultraviolet stable. A window make-up fitted flat is the single most common reason a skylight mists at ten or twelve years instead of twenty-five.

Why a sealed unit mists: the desiccant, the seal and the pressure cycle
The kerb is measured before anything is ordered.

Why a rooflight gets there before the windows in the same house

Householders often notice that the rooflights on an extension have gone cloudy while the windows fitted the same week are perfect. That is not bad luck and it is not a batch fault. Four things separate the two positions.

The first is water. A pane set at a shallow pitch sheds slowly, and the low edge of a flat rooflight holds a film of water against the very part of the unit that must stay dry. On a vertical window the same water is gone in seconds. The second is ultraviolet exposure, as above. The third is the thermal excursion already described. The fourth is debris: leaves, pine needles, moss and airborne grit collect on a horizontal surface and stay there, trapping moisture at the edge for weeks rather than hours.

None of that is a reason to avoid overhead glazing. It is a reason to specify overhead glazing as overhead glazing: silicone secondary seal, adequate edge cover, a genuine fall, and a warm-edge spacer.

The gas leaves before the water arrives

There is a second, quieter failure running in parallel. Argon molecules are small enough to permeate slowly through the secondary seal, and the fill drops gradually over the life of the unit. Nothing about this is visible. The rooflight looks perfect and performs a little worse every year.

Cavity fill What it is doing What happens over time
Air Nothing beyond separating the panes. The standard on most pre-2002 units No loss, because there is nothing to lose. The unit simply never performed well
Argon Denser than air, so it convects less across the cavity Permeates out slowly. A unit at the end of its life is measurably worse than the day it was made
Krypton Better still, and useful where the cavity has to be narrow Same slow loss, and it costs considerably more to put in

The practical point for a replacement is that the thermal gap between a 1990s unit and a current one is wider than the published figures suggest, because the old one has been leaking performance for two decades and was never tested again.

Failure is gradual, the symptom is sudden

Most people can date the misting to a particular fortnight, usually in autumn. What happened in that fortnight was not the seal breaking. It was the dew point inside the cavity crossing the temperature the glass was reaching at four in the morning. For a while the mist appears on cold nights and clears by lunchtime, which is why people convince themselves it is condensation in the room. As the desiccant saturates further, the mist stops clearing, and eventually a tide mark appears where liquid water has been standing at the low edge.

That progression is useful, because it means an early-stage failure gives you time. A misted unit is not an emergency. It is unattractive and it is costing you a little in heat, and it will get worse on its own schedule rather than suddenly.

Why a sealed unit mists: the desiccant, the seal and the pressure cycle
A prepared kerb, squared and weatherproofed, before the unit goes on.

What the mechanism tells you to put back

Understanding the failure changes the specification of the replacement, which is the only reason any of this matters commercially.

If a unit reached twenty or twenty-five years, it finished an ordinary life and a good current unit in the same position will do the same or better. If it reached ten or twelve, something in the original build-up was wrong for a roof: a polysulphide secondary seal under direct sun, edge cover shortened to make a slim frame look slimmer, a dead-flat setting that let the low edge stand in water, or a plain aluminium spacer driving a cold edge strip that condensed and kept the perimeter wet from the inside. Put the same thing back and you have bought the same failure on the same timetable.

Where Poole comes into the physics

Ultraviolet and salt are not the same attack, and the harbour gives you both. Ultraviolet degrades the secondary seal directly. Salt does not attack the sealant so much as everything holding the assembly in position: the fixings, the clips, the steel reinforcement inside a composite frame and the coating on the aluminium. On the spit at Sandbanks, with open water on both sides and no fetch break on the prevailing south-westerly, the two arrive together and a unit that would run twenty years at Broadstone is commonly finished by fifteen. Four miles inland the salt is simply not in the air, and specifying marine-grade components there is money spent on a threat that is not present. We will say so.

What we check before specifying the replacement

  1. Where the misting sits on the pane, and whether it clears during the day — which separates an early failure from an advanced one.
  2. The edge cover: how much frame actually overlaps the perimeter seal, measured rather than assumed.
  3. The spacer type visible through the glass, which tells us whether the original was warm-edge or plain aluminium.
  4. Any date or batch stamp on the spacer bar, and the toughening mark etched in a corner, which between them usually date the unit.
  5. Whether the low edge has a genuine fall, or whether water has been standing on the very seal that failed.
  6. The exposure zone the address sits in, which decides coating, fixings and whether marine specification is justified or an overcharge.

That produces a fixed written price rather than an estimate that moves once the old unit is out, and our installation work carries a ten-year workmanship guarantee given directly by us, which is not insurance backed. If your rooflight has gone cloudy and you want to know whether it failed early or simply finished, ring 01202 923272 and describe what you can see.

Get a fixed quote

Get a fixed quote

Tell us which way your roof faces.

We will come back with a specification, not a catalogue page. If your extension faces south we will tell you the G-value we would fit and why.

  • No pressure, no doorstep sales call
  • We handle the Building Control notification
  • 10-year workmanship guarantee on every installation
  • Installations and replacements across Poole and south Dorset

Prefer to talk it through? 01202 923272